:root { --theme-color:#ef4136; } .jz_theme_font_color { color: #ef4136; } .jz_theme_bg_color { background-color: #ef4136; } .jz_theme_border_color { border-color: #ef4136; } .jz_theme_fill_color { fill: #ef4136; } .jz_theme_focus_border_color:focus { border-color: #ef4136; } .jz_theme_hover_font_color:hover { color: #ef4136; } .pagination_style2 .pagination_item.active::after { border-color: #ef4136 !important; } .pagination_style3 .pagination_item.active, .pagination_style2 .pagination_item.active { color: #ef4136 !important; } .pagination_style3 .pagination_item.active::after, .pagination_style2 .pagination_item.active::before, .full_screen_row .pagination_style1 .pagination_item.active::after { background-color: #ef4136 !important; } .jz_hover.jz_theme_bg_hover_color:hover { background-color: #ef4136; } .jz_hover.jz_theme_font_hover_color:hover { color: #ef4136; } .jz_hover.jz_theme_border_hover_color:hover { border-color: #ef4136; } .jz_focus.jz_theme_focus_border_color:focus { border-color: #ef4136; } .jz_secondary_bg_color { background-color: #f28830; } .jz_screen_pc .submit_btn_style_1:hover .form_submit, .submit_btn_style_3:hover .form_submit { color: #ef4136; border-color: #ef4136; } .submit_btn_style_4 .form_submit, .submit_btn_style_5 .form_submit{ color: #ef4136; border-color: #ef4136; } .submit_btn_style_0 .form_submit,.submit_btn_style_1 .form_submit,.submit_btn_style_2 .form_submit { background-color: #ef4136; } .jz_screen_pc .submit_btn_style_4:hover .form_submit { background-color: #ef4136; } .jz_screen_pc .submit_btn_style_2:hover .form_submit { background-color: #e33d33; }

界面剂的施工工艺

2019-04-16 09:14

1、施工环境须干燥,相对湿度应小于70%, 通风良好。基面及环境的温度不应低于+5℃。

2、基面准备:基面应该干净、不松动、无灰尘,油脂、青苔、地毯胶等应清除掉, 松动及开裂部位应事先凿除并修补好。

3、搅拌:每袋粉料(20公斤)加10升的水(水:粉=0.5 :1),须用电动设备进行搅拌, 搅拌成均匀的稀浆状。

4、涂刷与干燥:用滚筒或毛刷把浆料涂刷到基面上,不能漏刷,然后让涂面干燥(约12小时)。

5、养护与成品保护:必须加强通风,自然养护即可,待浆料实干(表面变灰黑色)并确认完全封闭基面后,方可开展后续的工序。

6、工具的清洗 凝固的浆料很难清除。工具用后,应尽快用水清洗干净。

真冠建材,环保腻子,净味腻子,河南净味腻子,河南环保腻子,建材